Machinabiltiy Rating
Machinability Ratings - Stainless
| Grade |
Approximate Surf. Ft. Per Min. |
% Relative Speed Based on B-1112 as 100% |
|
Grade |
Approximate Surf. Ft. Per Min. |
% Relative Speed Based on B-1112 as 100% (165 SFM) |
| 302 |
70 |
40 |
420 |
85 |
50 |
| 302/304 "B" |
55 |
28 |
420 F |
125 |
68 |
| 303 |
150 |
75 |
430 |
110 |
66 |
| 303 High Tensile |
80 |
43 |
430 F |
150 |
75 |
| 304 |
70 |
40 |
431 |
80 |
48 |
| 304 L |
70 |
40 |
440 A |
65 |
40 |
| 309 |
60 |
36 |
440 C |
65 |
40 |
| 310 |
60 |
36 |
440 F Se |
80 |
48 |
| 316 |
60 |
22 |
446 |
60 |
36 |
| 316 "B" |
50 |
36 |
Custom 455 |
55 |
28 |
| 316 L |
60 |
36 |
PH-13-8 MO |
60 |
36 |
| 317-317 L |
60 |
36 |
15-5 PH |
75 |
45 |
| 321 |
60 |
20 |
17-4 PH |
75 |
45 |
| 330 |
45 |
36 |
17-4 PH "H1150" |
85 |
50 |
| 347 |
60 |
54 |
17-7 PH |
75 |
45 |
| 403 |
95 |
54 |
AM 355 |
72 |
42 |
| 410 |
95 |
75 |
Nitronic 40 |
50 |
22 |
| 416 Ann |
150 |
50 |
Nitronic 50 |
50 |
22 |
| 416 H.T. |
85 |
50 |
Nitronic 60 |
50 |
22 |
| 418 (Greek Ascoloy) |
96 |
50 |
Carp. 20 |
70 |
40 |
| |
|
Super Alloys - Electrical Steels |
| Grade |
Approximate Surf. Ft. Per Min. |
% Relative Speed Based on B-1112 as 100% |
|
Grade |
Approximate Surf. Ft. Per Min. |
% Relative Speed Based on B-1112 as 100% (165 SFM) |
| Maraging "300" |
60 |
36 |
|
Nickel "625" |
20 |
12 |
| A-286 |
54 |
28 |
|
718 |
20 |
12 |
| 4750 |
60 |
36 |
|
X-750 |
20 |
12 |
| L-605 |
15 |
9 |
|
INVAR 36 "FM" |
92 |
55 |
| Nickel "200" |
110 |
66 |
|
Waspaloy |
45 |
20 |
| Nickel "400" |
80 |
48 |
|
Alloy C (C-276) |
40 |
18 |
| Nickel "405" |
80 |
48 |
|
Alloy X |
45 |
20 |
| Nickel "K-500" |
60 |
36 |
|
Kovar |
60 |
22 |
| Nickel "600" |
50 |
22 |
|
Alloy R41 |
15 |
9 |
Download Machinability Rating (PDF - 96KB)